Walk into any columbarium and open a few doors to look at the carcass: nine times out of ten it is galvanised steel. This is not the industry cutting corners. It is the result of three conditions being met at once — the cost can be held down, the fabrication can be scaled, and the rust protection lasts Remove any one of the three and another material can take its place; so far, nothing else meets all three.

Cost. Galvanised coil runs about 1.2 times cold-rolled sheet and a third to a quarter of stainless. Carcass volume in a columbarium is not small: a two-hundred-niche hall consumes sheet by the tonne, so that multiple directly sets the price.
Workability. Galvanised sheet folds spot-welds and punches, and one set of dies can produce return flanges, stiffeners and door-frame folds. A columbarium carcass is a folded sheet-metal part, not a welded structural frame, and the fabrication method decides the material.
Rust protection. The zinc layer protects the cut edge by sacrificial action, and that is the core advantage over cold-rolled sheet. A columbarium is a high-humidity environment: a painted cold-rolled carcass shows rust at the cut edges within five years while galvanised lasts beyond ten.
Coating weight is the single most important parameter of a niche carcass, and the industry usually states it as "80 g/m² double-sided" — 80 grams across both faces. Converted to thickness: zinc has a density of 7.14, so 80 g/m² double-sided is 40 g/m² per face, about 5.6 microns.
5.6 microns sounds thin, but zinc corrodes at roughly 0.5 micron per year in a dry indoor environment and 1–1.5 microns per year when damp. That means an 80 g/m² coating lasts four to ten years inside a columbarium before white rust begins. It is also why the inside of some older carcasses carries a layer of white powder — that is zinc corroding.
The next step up is 120–180 g/m² (8–12 microns per face), which doubles the life for about 15% more cost. Humid regions, bottom tiers and external-wall niches are worth the upgrade.
Galvanised protection is a global coating plus local sacrifice, but two locations fail first:
Cut edges. The sheared or punched section has no zinc; it is bare steel. It is protected by the surrounding zinc sacrificing itself, but that protection reaches only 1–2 mm. Carcasses with many cut openings — lots of ventilation holes, for example — start rusting at the hole edges.
Welds. Spot welding burns the coating away, leaving a 3–5 mm zinc-free zone around each weld. Zinc also melts at 419°C and vaporises during welding, leaving porosity in the weld — and that porosity is a doorway for moisture.
The correct practice is to grind cut edges and welds and apply zinc-rich paint, restoring the sacrificial capability. Done in the factory this costs very little; not done, it shows in three to five years.

Look at a cut section. If the sheared edge is bright with no grey-white layer, the coating is thin or absent. A proper galvanised edge shows a clear grey-white skin.
Look for white rust. White powdery deposit on the inside of the carcass is the product of zinc corrosion, and it means the coating is being consumed.
Ask for the specification. A proper manufacturer can state coating weight in g/m² and sheet thickness. Anyone who says only "galvanised" without a number should be assumed to be at the bottom grade.
Feel a folded corner. The coating on the outside of a fold is stretched thinner. If it feels noticeably rough under your thumb, the coating is on the light side.
Three cases:
One: bottom tier and external-wall niches. These are the wettest, most condensation-prone positions, where the coating is consumed at more than double the rate. Specify stainless or a heavier coating.
Two: coastal high-salt regions. Chloride accelerates zinc corrosion and halves the life of ordinary galvanised sheet. Specify 304 stainless or aluminium.
Three: niches that must be maintenance-free long term. The maintenance cycle for galvanised is 8–10 years (touch-up painting, removing white rust). If the operator lacks the capacity to maintain, paying more up front is actually cheaper.
The greatest risk in material selection is applying one answer to everything. In the same hall, the row against the external wall and the middle row live in very different conditions; using one material for both means one of them ages early.
Q: Should the inside of a galvanised carcass be painted?
A: Yes, recommended. The coating does not touch the ashes, but white rust powder falls. A coat of water-based anti-rust paint on the inner face both isolates and tidies it.
Q: Is a thicker coating always better?
A: Within reason. Beyond about 275 g/m² the coating tends to crack and flake when folded, and workability drops.
Q: How do I tell galvanised from stainless by eye?
A: Galvanised has spangle — a crystalline pattern — and reads grey-white; stainless reads bright silver with no spangle. A magnet also helps: galvanised is strongly magnetic, 304 weakly so.

Galvanised became the standard because it found the balance point between cost, fabrication and rust protection. It is not a universal material: cut edges need paint, welds need treatment, and the bottom tier and external wall need an upgrade. The carcass is the skeleton of the niche, so when specifying, one extra question about coating weight in grams is worth more than another glossy brochure.